Causes and preventive measures of crack defects caused by high-frequency heating machine heat treatment of workpieces

2021-12-22 8:34:22

RIO Technology 溫州瑞奧科技有限公司
Share
  • Share to WeChat Moments

Gears, half shafts, camshafts, and connecting rods are usually heat treated by high-frequency heating machines. During the heat treatment process, affected by various factors, some defects will occur, such as cracks, decarburization, and unqualified hardness.



Today, let's explore the cracks in the workpiece during the heat treatment process, which are caused by improper process operations, and how should we solve them?

1. Poor cooling or uneven cooling, causes of poor cooling or uneven cooling and preventive measures are as follows:

1. The structure of the sprayer is poorly designed, we need to improve the design of the sprayer;

2. If the quenching cooling medium is not properly selected, we should choose the appropriate quenching cooling medium to control the critical cooling rate and the cooling rate of the martensite section;

3. Improper formulation or management of quenching cooling medium regulations (improper maintenance of concentration, flow rate, time, and sprayer), we need to improve the formulation and implementation of cooling regulations.



2. Uneven heating temperature or overheating, the causes and solutions are as follows:

1. The electrical specification of the heating device is out of control, the power is too large or the heating time is too long. For this, we should correct the shortcomings of the control system;

2. The relative position of the workpiece and the sensor is incorrect, and the operation sequence is wrong. We should strictly operate the process rules for the problem;

3. The inductor of the high-frequency heating machine is poorly designed and manufactured, resulting in uneven temperature or overheating locally. We should improve the design and manufacturing quality of the inductor.




3. Poor tempering Reasons and preventive measures for poor tempering are as follows:

1. Normalizing or high temperature tempering is not carried out during repair, and the repaired parts need to be normalized or tempered at high temperature;

2. If it is not tempered in time after quenching, we should temper it in time after quenching;

3. If the tempering heating speed and temperature are not appropriate, we should adopt the correct tempering heating speed and temperature to ensure that the process requirements are met.


 

高頻加熱機(jī)

 

Keywords: high frequency heating machine

Note: The above information is organized and released by Wenzhou Ruiao Technology Co., Ltd. (www.cncnr.cn)


HOME About Us Product News Case Video Advantages Contact
主站蜘蛛池模板: 一级做a爱片久久毛片a片v | 色吊丝中文字幕一区二区三区 | 最新手机在线电影电 | 97精品免视看秋霞 | 中文字幕一区不卡更新二区 | 中文无码一区二区不卡αv 中文无码一区二区三区不卡av | 亚洲人成伊人成综合网中文 | 亚洲v午夜精品无码专区 | 在线视频观看 | 中文字幕精品亚洲一区 | 日韩亚洲欧美高清一区二区久 | 国产自产在线观看 | 狠狠噜天天噜日日噜 | 亚洲国产日韩a在线乱码 | 91制片厂制作果冻星空传媒 | 亚洲av无码精品国产天堂 | 国产综合丝袜高跟在线 | 国产乱子伦一区二区三区 | 特黄大片 | 91精品国产综合久久福利 | 亚洲中文字幕精品久久久久久动漫 | 国产成人免费av片在线观看婷婷 | 天天干狠狠操 | 亚洲精品美女久久久久99 | 少妇无码av无码去区钱 | 丰满少妇女人a毛片视频 | 国产交换配乱婬视频手机版 | 国产在线精品一区二区三区直 | 亚洲精品成人片在线播放 | 91pao对白在线播放 | 东京无码熟妇人妻av在线 | 日产精品一区二区三区免费 | 国产精品巨作av无 | 人妻精品久久久久中文字幕 | 亚洲av永久无码精品秋霞电影 | 深夜福利小视频 | 一区二区三区日本精品 | 91精品人妻一区二区三区 | 欧美重变态videos乱 | 91秒拍国产福利片 | 亚洲欧美日韩另类精品一区二区三区 |